CBIES AUTOMOTIVE|The Reason For The Eccentricity (uneven Thickness) Of Seamless Steel Pipe Production
The finished products of seamless steel pipes and precision steel pipes will have the problem of uneven eccentric thickness, but how does it happen? Many people don't understand, today CBIES will explain how the eccentricity of seamless steel pipes such as cold-drawn steel pipes, cold-rolled steel pipes, and hot-rolled steel pipes is produced, and why the concentricity of seamless steel pipes is not so ideal.
Eccentric steel pipes are most likely to occur in the production process of hot-rolled steel pipes, and most of the links are generated during hot piercing:
According to the anatomical analysis of the steel pipe rolled by the automatic pipe rolling machine, we believe that after the perforated capillary pipe is rolled by the automatic pipe rolling machine, the uneven wall thickness of the steel pipe in the vertical and horizontal directions basically retains the distribution characteristics of the uneven wall thickness of the perforated capillary pipe. That is, the steel pipe still has spiral uneven wall thickness after rolling, and the transverse wall thickness unevenness increases significantly.
The reasons for the uneven wall thickness of the automatic pipe rolling mill are:
A.The existence form and severity of the uneven wall thickness of the perforated capillary directly affect the existing form and severity of the uneven wall thickness of the rolled steel pipe.
B. When the pipe is rolled on the automatic pipe rolling machine, due to the bending of the ejector rod, the position of the plug deviates from the center of the pass, resulting in uneven wall thickness. However, the degree of wall thickness unevenness from the end of the pipe to the head of the pipe gradually increases. Therefore, reducing the residual curvature of the ejector rod and reducing the axial force of the ejector rod during pipe rolling have an effect on reducing the degree of wall thickness unevenness. significant effect.
C. The greater the amount of wall reduction, the more serious the uneven wall thickness of the waste pipe. When the amount of wall reduction is small, the automatic pipe rolling machine can reduce the uneven wall thickness of the perforated capillary tube.
D. The pass adjustment is not correct. When the roll gap is not parallel, the uneven wall thickness of the waste pipe will be aggravated.
CBIES AUTOMOTIVE has been deeply involved in the auto parts industry for many years. For the treatment of seamless pipe wall thickness deviation, the perforation technology at the source is refined. It has excellent perforation equipment. The furnace is equipped with preheating, heating, and high-temperature zones, and natural gas nozzles are used throughout. , uniform temperature to ensure the quality of perforation. Make random inspection records during the whole process of piercing, and inspect the capillary root after piercing to ensure the quality of the capillary.
Finish-rolled steel pipes and cold-drawn steel pipes also have eccentricity problems due to perforation:
Any factor that destroys the geometrical correctness of the deformation zone formed by the roll, the plug, and the guide plate will aggravate the uneven wall thickness of the capillary.
A. Head
(a) The shape design of the plug. The ideal rolling cone of the plug should be parallel to the exit cone of the roll. If the plug is designed according to the traditional Matveyev formula, the rolling cone of the plug is not parallel to the exit cone of the roll. The deformation of the metal in such a gradually expanding gap will inevitably lead to insufficient rolling of the tube wall, resulting in uneven wall thickness of the capillary tube, and the uneven wall thickness of the capillary tube will become more serious with the increase of the feeding angle;
(b) Due to the insufficient rigidity of the ejector rod, it is bent during the piercing process, so that the plug cannot maintain the centered position, so that the thickness of the capillary tube that passes through is uneven;
(c) Uneven wear or damage to the plug.
B. Guide plate
(a) The guide plate distance is too large. During the perforation process, the center line of the perforation is maintained by the restriction of the guide plate. If the guide plate distance is large, the position of the plug changes greatly, making the plug unstable, and resulting in uneven wall thickness of the capillary.
(b) The uneven wear of the upper and lower guide plates will also aggravate the uneven wall thickness.
roll
(a) Roll center line deflection: During the production process, due to incorrect installation of the pressing screws on both sides of the piercing machine, or due to thread and bearing wear, the axial direction between the two rolls is horizontally deflected, and the feeding of the two rolls Angle inconsistency distorts the deformation zone resulting in uneven wall thickness.
(b) The rolling cone of the plug and the roll is more non-parallel under the large feed angle.
(c) Improper roll speed will also affect the wall thickness accuracy.
C. Centering and heating of the tube blank
Both eccentric centering holes and uneven heating (male and female sides) will cause varying wall thickness.
D. Rigidity, structure, and adjustment of the punching machine
The rigidity of the body of the piercing machine is not enough, and the locking mechanism on it is unreliable; the centering device of the ejector rod is not adjusted accurately, the operation is unreliable and the distance from the body is far; the adjustment of the rolling center line is generally lower than the center line of the rolling mill. , the purpose is to improve the stability of the rolled piece. If the adjustment is too large, the relative relationship between the tools in the deformation zone will change asymmetrically after the rolling line moves down, which will also affect the uneven wall thickness of the capillary.
Therefore, there is no way to altogether avoid the uneven eccentric thickness of seamless steel pipes, and it can only be strictly controlled step by step to minimize